Mitsubishi Chemical Advanced Materials TIVAR™ 1000 Colors UHMW-PE
Categories: Polymer; Thermoplastic; Polyethylene (PE); UHMW-PE

Material Notes: TIVAR™ 1000 colors Ultra High Molecular Weight Polyethylene UHMW-PE shapes have a well-balanced property profile with a unique combination of wear and corrosion resistance, a low friction surface, excellent impact strength, and FDA-compliant composition.

Printer friendly version Printer friendly version  PDF Download Download as PDF  Add to Folder:
 
Physical PropertiesMetricEnglishComments
Specific Gravity 0.930 g/cc0.930 g/ccASTM D792
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 60.060.0ISO 868
Tensile Strength 19.0 MPa2760 psiISO 527-1/-2 (7)
Elongation at Yield 15.0 %15.0 %ISO 527-1/-2 (7)
Flexural Strength 17.0 MPa2470 psiISO 178 (12)
Compressive Yield Strength  6.50 MPa
@Strain 1.00 %
943 psi
@Strain 1.00 %
ISO 604 (10)
 10.5 MPa
@Strain 2.00 %
1520 psi
@Strain 2.00 %
ISO 604 (10)
 17.0 MPa
@Strain 5.00 %
2470 psi
@Strain 5.00 %
ISO 604 (10)
Shear Strength 33.0 MPa4790 psiASTM D732
Charpy Impact, Notched 11.5 J/cm²54.7 ft-lb/in²Partial Break; ISO 179-1/1eA
 17.0 J/cm²80.9 ft-lb/in²Double Notched
 
Electrical PropertiesMetricEnglishComments
Surface Resistivity per Square 1.00e+14 ohm1.00e+14 ohmANSI/ESD STM 11.11
Dielectric Constant 2.30
@Frequency 1.00e+6 Hz
2.30
@Frequency 1.00e+6 Hz
ASTM D150
Dielectric Strength 45.0 kV/mm1140 kV/inIEC 60243-1 (15)
 45.3 kV/mm1150 kV/inASTM D149
Dissipation Factor 0.000500
@Frequency 1.00e+6 Hz
0.000500
@Frequency 1.00e+6 Hz
ASTM D150
 
Thermal PropertiesMetricEnglishComments
CTE, linear 198 µm/m-°C110 µin/in-°FASTM E-831 (TMA)
 200 µm/m-°C
@Temperature 23.0 - 100 °C
111 µin/in-°F
@Temperature 73.4 - 212 °F
Thermal Conductivity 0.400 W/m-K2.78 BTU-in/hr-ft²-°F
 0.409 W/m-K2.84 BTU-in/hr-ft²-°F
Melting Point 135 °C275 °FASTM D3418
Maximum Service Temperature, Air 82.2 °C180 °FContinuous Use Temperature in Air after 20000 hr
Deflection Temperature at 1.8 MPa (264 psi) 46.7 °C116 °FASTM D648
Minimum Service Temperature, Air -200 °C-328 °F
 
Compliance PropertiesMetricEnglishComments
FDA YesYes
 
Chemical Resistance PropertiesMetricEnglishComments
Acids, Strong (pH 1-3) AcceptableAcceptable
Acids, Weak AcceptableAcceptable
Alcohols AcceptableAcceptable
Alkalies, Strong (pH 11-14) AcceptableAcceptable
Alkalies, Weak AcceptableAcceptable
Chlorinated Solvents AcceptableAcceptable
Continuous Sunlight LimitedLimited
Hot Water / Steam LimitedLimited
Hydrocarbons - Aliphatic AcceptableAcceptable
Hydrocarbons - Aromatic AcceptableAcceptable
Inorganic Salt Solutions AcceptableAcceptable
Ketones, Esters AcceptableAcceptable
 
Miscellaneous PropertiesMetricEnglishComments
Targeted Usage Load + BearingLoad + Bearing
 
Descriptive Properties
ESd categoryInsulative

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.