Mitsubishi Chemical Advanced Materials Nylatron™ 101 / Ertalon™ 66 SA PA66 Extruded, Unfilled, Type 66 Natural and Black
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, Extruded

Material Notes: A high mechanical strength, fatigue resistant nylon 66 with excellent wear resistance and electrical insulating properties.

Key Words: Polyamide 66; PA66; PA 66; Polyamide 6/6; Polyamide 6,6; Nylon 6/6; Nylon 6,6
Printer friendly version Printer friendly version  PDF Download Download as PDF  Add to Folder:
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.15 g/cc1.15 g/ccASTM D792
Water Absorption at Saturation 7.00 %7.00 %ASTM D570 (17)
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 88.088.0ASTM D785
Hardness, Shore D 80.080.0ISO 868
Tensile Strength 90.0 MPa13100 psiISO 527-1/-2 (7)
Elongation at Yield 5.00 %5.00 %ISO 527-1/-2 (7)
Flexural Strength 135 MPa19600 psiISO 178 (12)
Compressive Yield Strength  32.0 MPa
@Strain 1.00 %
4640 psi
@Strain 1.00 %
ISO 604 (10)
 62.0 MPa
@Strain 2.00 %
8990 psi
@Strain 2.00 %
ISO 604 (10)
 100 MPa
@Strain 5.00 %
14500 psi
@Strain 5.00 %
ISO 604 (10)
Shear Strength 69.0 MPa10000 psiASTM D732
Charpy Impact, Notched 0.450 J/cm²2.14 ft-lb/in²ISO 179-1/1eA
 
Electrical PropertiesMetricEnglishComments
Surface Resistivity per Square 1.00e+14 ohm1.00e+14 ohmANSI/ESD STM 11.11
Dielectric Constant 3.60
@Frequency 1.00e+6 Hz
3.60
@Frequency 1.00e+6 Hz
ASTM D150
Dielectric Strength 15.7 kV/mm400 kV/inASTM D149
 27.0 kV/mm686 kV/inIEC 60243-1 (15)
Dissipation Factor 0.0200
@Frequency 1.00e+6 Hz
0.0200
@Frequency 1.00e+6 Hz
ASTM D150
 
Thermal PropertiesMetricEnglishComments
CTE, linear 99.0 µm/m-°C55.0 µin/in-°FASTM E-831 (TMA)
 80.0 µm/m-°C
@Temperature 23.0 - 60.0 °C
44.4 µin/in-°F
@Temperature 73.4 - 140 °F
 95.0 µm/m-°C
@Temperature 23.0 - 100 °C
52.8 µin/in-°F
@Temperature 73.4 - 212 °F
Thermal Conductivity 0.245 W/m-K1.70 BTU-in/hr-ft²-°F
 0.280 W/m-K1.94 BTU-in/hr-ft²-°F
Melting Point 260 °C500 °FASTM D3418
Maximum Service Temperature, Air 79.4 °C175 °FContinuous Use Temperature in Air after 20000 hr
Deflection Temperature at 1.8 MPa (264 psi) 93.3 °C200 °FASTM D648
Minimum Service Temperature, Air -30.0 °C-22.0 °F
 
Chemical Resistance PropertiesMetricEnglishComments
Acids, Strong (pH 1-3) UnacceptableUnacceptable
Acids, Weak LimitedLimited
Alcohols LimitedLimited
Alkalies, Strong (pH 11-14) UnacceptableUnacceptable
Alkalies, Weak LimitedLimited
Chlorinated Solvents LimitedLimited
Continuous Sunlight LimitedLimited
Hot Water / Steam LimitedLimited
Hydrocarbons - Aliphatic AcceptableAcceptable
Hydrocarbons - Aromatic AcceptableAcceptable
Inorganic Salt Solutions AcceptableAcceptable
Ketones, Esters AcceptableAcceptable
 
Miscellaneous PropertiesMetricEnglishComments
Data Sheet Region AmericasAmericas
Targeted Usage Load + BearingLoad + Bearing
 
Descriptive Properties
ESd categoryInsulative

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.