Physical PropertiesMetricEnglishComments
Specific Gravity 1.40 g/cc1.40 g/ccASTM D792
Water Absorption at Saturation 1.70 %1.70 %ASTM D570 (17)
 
Electrical PropertiesMetricEnglishComments
Surface Resistivity per Square 1.00e+14 ohm1.00e+14 ohmANSI/ESD STM 11.11
Dielectric Constant 4.20
@Frequency 1.00e+6 Hz
4.20
@Frequency 1.00e+6 Hz
ASTM D150
Dielectric Strength 22.8 kV/mm580 kV/inASTM D149
Dissipation Factor 0.0260
@Frequency 1.00e+6 Hz
0.0260
@Frequency 1.00e+6 Hz
ASTM D150
 
Thermal PropertiesMetricEnglishComments
CTE, linear 30.6 µm/m-°C17.0 µin/in-°FASTM E-831 (TMA)
Thermal Conductivity 0.259 W/m-K1.80 BTU-in/hr-ft²-°F
Maximum Service Temperature, Air 260 °C500 °FContinuous Use Temperature in Air after 20000 hr
Deflection Temperature at 1.8 MPa (264 psi) 278 °C532 °FASTM D648
Glass Transition Temp, Tg 275 °C527 °FDMA- Tan d
 
Chemical Resistance PropertiesMetricEnglishComments
Acids, Strong (pH 1-3) LimitedLimited
Acids, Weak AcceptableAcceptable
Alcohols AcceptableAcceptable
Alkalies, Strong (pH 11-14) UnacceptableUnacceptable
Alkalies, Weak LimitedLimited
Chlorinated Solvents AcceptableAcceptable
Continuous Sunlight AcceptableAcceptable
Hot Water / Steam LimitedLimited
Hydrocarbons - Aliphatic AcceptableAcceptable
Hydrocarbons - Aromatic AcceptableAcceptable
Inorganic Salt Solutions AcceptableAcceptable
Ketones, Esters AcceptableAcceptable
 
Miscellaneous PropertiesMetricEnglishComments
Data Sheet Region AmericasAmericas
Targeted Usage Load + BearingLoad + Bearing
 
Descriptive Properties
ESd categoryInsulative

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

P1SM34e / 89258