Mitsubishi Chemical Advanced Materials Ketron™ VMX FG PEEK Food Grade Polyetheretherketone
Categories: Polymer; Thermoplastic; Polyketone; Polyetheretherketone (PEEK); Polyetheretherketone, PEEK, Unreinforced

Material Notes: A metal-detectable PEEK with FDA and EU compliance that offers extreme dimensional stability, high strength, and temperature resistance.

Printer friendly version Printer friendly version  PDF Download Download as PDF  Add to Folder:
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.45 g/ccASTM D792
Water Absorption at Saturation 0.210 %ASTM D570 (17)
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 106ASTM D785
Tensile Strength 114 MPaISO 527-1/-2 (7)
Elongation at Yield 4.00 %ISO 527-1/-2 (7)
Compressive Yield Strength 45.0 MPa
@Strain 1.00 %
ISO 604 (10)
 86.0 MPa
@Strain 2.00 %
ISO 604 (10)
 144 MPa
@Strain 5.00 %
ISO 604 (10)
Shear Strength 83.0 MPaASTM D732
Charpy Impact, Notched 3.20 kJ/m²ISO 179-1/1eA
 
Thermal PropertiesOriginal ValueComments
CTE, linear 25.0 µin/in-°FASTM E-831 (TMA)
 45.0 µm/m-°C
@Temperature 23.0 - 100 °C
Thermal Conductivity 1.73 BTU-in/hr-ft²-°F
Melting Point 644 °FASTM D3418
Maximum Service Temperature, Air 480 °FContinuous Use Temperature in Air after 20000 hr
Deflection Temperature at 1.8 MPa (264 psi) 320 °FASTM D648
 
Compliance PropertiesOriginal ValueComments
FDA Yes
 
Chemical Resistance PropertiesOriginal ValueComments
Acids, Strong (pH 1-3) Limited
Acids, Weak Acceptable
Alcohols Acceptable
Alkalies, Strong (pH 11-14) Acceptable
Alkalies, Weak Acceptable
Chlorinated Solvents Acceptable
Continuous Sunlight Limited
Hot Water / Steam Acceptable
Hydrocarbons - Aliphatic Acceptable
Hydrocarbons - Aromatic Acceptable
Inorganic Salt Solutions Acceptable
Ketones, Esters Acceptable

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.