Mitsubishi Chemical Advanced Materials Duratron™ T4203 PAI Extruded Polyamide-imide
Categories: Polymer; Thermoplastic; Polyamide-imide (PAI); Polyamide-Imide, Extruded

Material Notes: The ultimate PAI for impact strength and elongation, can bear high loads in extreme temperatures and offers exceptional dimensional stability and machinability.

Printer friendly version Printer friendly version  PDF Download Download as PDF  Add to Folder:
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.41 g/ccASTM D792
Water Absorption at Saturation 1.70 %ASTM D570 (17)
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell E 80.0ASTM D785
Hardness, Shore D 88.0ISO 868
Tensile Strength 150 MPaISO 527-1/-2 (7)
Elongation at Yield 9.00 %ISO 527-1/-2 (7)
Flexural Strength 178 MPaISO 178 (12)
Compressive Yield Strength 34.0 MPa
@Strain 1.00 %
ISO 604 (10)
 67.0 MPa
@Strain 2.00 %
ISO 604 (10)
 135 MPa
@Strain 5.00 %
ISO 604 (10)
Shear Strength 110 MPaASTM D732
Charpy Impact, Notched 15.0 kJ/m²ISO 179-1/1eA
 
Electrical PropertiesOriginal ValueComments
Surface Resistivity per Square 1.00e+14 ohmANSI/ESD STM 11.11
Dielectric Constant 4.20
@Frequency 1.00e+6 Hz
ASTM D150
Dielectric Strength 24.0 kV/mmIEC 60243-1 (15)
 580 kV/inASTM D149
Dissipation Factor 0.0260
@Frequency 1.00e+6 Hz
ASTM D150
 
Thermal PropertiesOriginal ValueComments
CTE, linear 21.0 µin/in-°FASTM E-831 (TMA)
 40.0 µm/m-°C
@Temperature 23.0 - 100 °C
 40.0 µm/m-°C
@Temperature 23.0 - 150 °C
 50.0 µm/m-°C
@Temperature >=150 °C
Thermal Conductivity 0.260 W/m-K
 1.80 BTU-in/hr-ft²-°F
Maximum Service Temperature, Air 500 °FContinuous Use Temperature in Air after 20000 hr
Deflection Temperature at 1.8 MPa (264 psi) 532 °FASTM D648
Minimum Service Temperature, Air -50.0 °C
Glass Transition Temp, Tg 527 °FDMA- Tan d
 
Chemical Resistance PropertiesOriginal ValueComments
Acids, Strong (pH 1-3) Limited
Acids, Weak Acceptable
Alcohols Acceptable
Alkalies, Strong (pH 11-14) Unacceptable
Alkalies, Weak Limited
Chlorinated Solvents Acceptable
Continuous Sunlight Limited
Hot Water / Steam Limited
Hydrocarbons - Aliphatic Acceptable
Hydrocarbons - Aromatic Acceptable
Inorganic Salt Solutions Acceptable
Ketones, Esters Acceptable
 
Miscellaneous PropertiesOriginal ValueComments
Data Sheet Region Americas
Targeted Usage Structural Uses
 
Descriptive Properties
ESd categoryInsulative

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.