System Message
Searches:
Step-by-Step Selector
|
Quick Database Search
Mitsubishi Chemical Advanced Materials Fluorosint™ 135 PTFE and PPS Blend, with Proprietary Lubrication Fillers
Categories:
Polymer
;
Thermoplastic
;
Fluoropolymer
;
Polytetrafluoroethylene (PTFE)
;
Polyphenylene Sulfide (PPS)
Material Notes:
Formulated to provide the lowest coefficient of friction and deformation for use in seal, bearing, and washer applications, this PTFE also exhibits excellent strength, stiffness, and high-pressure velocity capabilities.
Printer friendly version
Download as PDF
Add to Folder:
My Folder
-- task --
Export to Solidworks
Export to ALGOR
Export to ANSYS
Export to NEiWorks
Export to COMSOL
Export to ETBX
Export to SpaceClaim
Physical Properties
Metric
English
Comments
Specific Gravity
1.91
g/cc
1.91
g/cc
ASTM D792
Water Absorption at Saturation
0.300 %
0.300 %
ASTM D570 (17)
Mechanical Properties
Metric
English
Comments
Hardness, Rockwell R
67.0
67.0
ASTM D785
Tensile Strength
11.0
MPa
1600
psi
ISO 527-1/-2 (7)
Elongation at Yield
3.00 %
3.00 %
ISO 527-1/-2 (7)
Compressive Yield Strength
19.0
MPa
@Strain 1.00 %
2760
psi
@Strain 1.00 %
ISO 604 (10)
25.0
MPa
@Strain 2.00 %
3630
psi
@Strain 2.00 %
ISO 604 (10)
30.0
MPa
@Strain 5.00 %
4350
psi
@Strain 5.00 %
ISO 604 (10)
Shear Strength
17.0
MPa
2470
psi
ASTM D732
Charpy Impact, Notched
0.350
J/cm²
1.67
ft-lb/in²
ISO 179-1/1eA
Electrical Properties
Metric
English
Comments
Surface Resistivity per Square
1e+05
1e+05
ANSI/ESD STM 11.11
Thermal Properties
Metric
English
Comments
CTE, linear
45.0
µm/m-°C
25.0
µin/in-°F
ASTM E-831 (TMA)
50.0
µm/m-°C
@Temperature 23.0 - 100 °C
27.8
µin/in-°F
@Temperature 73.4 - 212 °F
55.0
µm/m-°C
@Temperature 23.0 - 150 °C
30.6
µin/in-°F
@Temperature 73.4 - 302 °F
85.0
µm/m-°C
@Temperature >=150 °C
47.2
µin/in-°F
@Temperature >=302 °F
Melting Point
327
°C
621
°F
ASTM D3418
Maximum Service Temperature, Air
260
°C
500
°F
Continuous Use Temperature in Air after 20000 hr
Deflection Temperature at 1.8 MPa (264 psi)
104
°C
220
°F
ASTM D648
Minimum Service Temperature, Air
-50.0
°C
-58.0
°F
Chemical Resistance Properties
Metric
English
Comments
Acids, Strong (pH 1-3)
Acceptable
Acceptable
Acids, Weak
Acceptable
Acceptable
Alcohols
Acceptable
Acceptable
Alkalies, Strong (pH 11-14)
Acceptable
Acceptable
Alkalies, Weak
Acceptable
Acceptable
Chlorinated Solvents
Acceptable
Acceptable
Continuous Sunlight
Acceptable
Acceptable
Hot Water / Steam
Acceptable
Acceptable
Hydrocarbons - Aliphatic
Acceptable
Acceptable
Hydrocarbons - Aromatic
Acceptable
Acceptable
Inorganic Salt Solutions
Acceptable
Acceptable
Ketones, Esters
Acceptable
Acceptable
Descriptive Properties
ESd category
Dissipative
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
P1SM08w / 137230