Mitsubishi Chemical Advanced Materials Semitron™ ESd 225 POM Extruded, Static Dissipative Acetal
Categories: Polymer; Thermoplastic; Acetal (Polyoxymethylene, POM); Acetal Copolymer, Unreinforced

Material Notes: A line of POM shapes characterized by excellent wear resistance, thermal performance, and quick dissipation of static charges. Due to these properties, this grade is ideal for several applications throughout the semiconductor and electronics industry.

Key Words: POM, Polyoxymethylene; Polyformaldehyde; Polyacetal
Printer friendly version Printer friendly version  PDF Download Download as PDF  Add to Folder:
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.33 g/ccASTM D792
Water Absorption at Saturation 8.00 %ASTM D570 (17)
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 106ASTM D785
Hardness, Shore D 75.0ISO 868
Tensile Strength 38.0 MPaISO 527-1/-2 (7)
Flexural Strength 50.0 MPaISO 178 (12)
Compressive Yield Strength 14.0 MPa
@Strain 1.00 %
ISO 604 (10)
 25.0 MPa
@Strain 2.00 %
ISO 604 (10)
 38.0 MPa
@Strain 5.00 %
ISO 604 (10)
Shear Strength 41.0 MPaASTM D732
Charpy Impact, Notched 8.00 kJ/m²ISO 179-1/1eA
 
Electrical PropertiesOriginal ValueComments
Surface Resistivity per Square 1.00e+10 - 1.00e+12 ohmANSI/ESD STM 11.11
Dielectric Constant 4.31
@Frequency 1.00e+6 Hz
ASTM D150
Dissipation Factor 0.0360
@Frequency 1.00e+6 Hz
ASTM D150
 
Thermal PropertiesOriginal ValueComments
CTE, linear 93.0 µin/in-°FASTM E-831 (TMA)
 150 µm/m-°C
@Temperature 23.0 - 100 °C
Melting Point 320 °FASTM D3418
Maximum Service Temperature, Air 190 °FContinuous Use Temperature in Air after 20000 hr
Deflection Temperature at 1.8 MPa (264 psi) 225 °FASTM D648
Minimum Service Temperature, Air -50.0 °C
 
Chemical Resistance PropertiesOriginal ValueComments
Acids, Strong (pH 1-3) Limited
Acids, Weak Limited
Alcohols Acceptable
Alkalies, Strong (pH 11-14) Acceptable
Alkalies, Weak Acceptable
Chlorinated Solvents Acceptable
Continuous Sunlight Acceptable
Hot Water / Steam Limited
Hydrocarbons - Aliphatic Acceptable
Hydrocarbons - Aromatic Unacceptable
Inorganic Salt Solutions Acceptable
Ketones, Esters Limited
 
Miscellaneous PropertiesOriginal ValueComments
Data Sheet Region Americas
Targeted Usage Structural Uses
 
Descriptive Properties
ESd categoryDissipative

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.