Mitsubishi Chemical Advanced Materials Duratron™ D7015G PI Bearing Grade Polyimide
Categories: Polymer; Thermoplastic; Polyimide, Thermoplastic

Material Notes: This hot compression molded, 15% graphite filled PI is a bearing grade material with superior temperature and wear resistance, as well as a low coefficient of friction.

Printer friendly version Printer friendly version  PDF Download Download as PDF  Add to Folder:
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.45 g/ccASTM D792
Water Absorption at Saturation 3.00 %ASTM D570 (17)
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 115ASTM D785
Hardness, Shore D 86.0ISO 868
Tensile Strength 105 MPaISO 527-1/-2 (7)
Flexural Strength 150 MPaISO 178 (12)
Compressive Yield Strength 40.0 MPa
@Strain 1.00 %
ISO 604 (10)
 70.0 MPa
@Strain 2.00 %
ISO 604 (10)
 130 MPa
@Strain 5.00 %
ISO 604 (10)
Shear Strength 90.0 MPaASTM D732
Charpy Impact, Notched 4.00 kJ/m²ISO 179-1/1eA
 
Electrical PropertiesOriginal ValueComments
Surface Resistivity per Square 10000 ohmANSI/ESD STM 11.11
Dielectric Strength 13.0 kV/mmIEC 60243-1 (15)
 
Thermal PropertiesOriginal ValueComments
CTE, linear 35.0 µin/in-°FASTM E-831 (TMA)
 37.0 µm/m-°C
@Temperature 23.0 - 100 °C
 40.0 µm/m-°C
@Temperature 23.0 - 150 °C
 49.0 µm/m-°C
@Temperature >=150 °C
Thermal Conductivity 0.390 W/m-K
 2.70 BTU-in/hr-ft²-°F
Maximum Service Temperature, Air 570 °FContinuous Use Temperature in Air after 20000 hr
Minimum Service Temperature, Air -321 °F
 -196 °C
Glass Transition Temp, Tg 735 °FDMA- Tan d
 
Chemical Resistance PropertiesOriginal ValueComments
Acids, Strong (pH 1-3) Acceptable
Acids, Weak Acceptable
Alcohols Acceptable
Alkalies, Strong (pH 11-14) Acceptable
Alkalies, Weak Acceptable
Chlorinated Solvents Unacceptable
Continuous Sunlight Limited
Hot Water / Steam Limited
Hydrocarbons - Aliphatic Unacceptable
Hydrocarbons - Aromatic Unacceptable
Inorganic Salt Solutions Acceptable
Ketones, Esters Unacceptable
 
Miscellaneous PropertiesOriginal ValueComments
Data Sheet Region Americas
Targeted Usage Load + Bearing
 
Descriptive Properties
ESd categoryConductive

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.