Mitsubishi Chemical Advanced Materials TIVAR™ VMX FG UHMW-PE Food Grade Ultra High Molecular Weight Polyethylene
Material Notes: A metal-detectable, food-grade polyethylene specifically developed to serve as a wear- and abrasion-resistant material with easy traceability in the food processing and packaging industries.

Printer friendly version Printer friendly version  PDF Download Download as PDF  Add to Folder:
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.07 g/ccASTM D792
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 62.0ISO 868
Tensile Strength 20.0 MPaISO 527-1/-2 (7)
Elongation at Yield 16.0 %ISO 527-1/-2 (7)
Flexural Strength 20.0 MPaISO 178 (12)
Compressive Yield Strength 7.00 MPa
@Strain 1.00 %
ISO 604 (10)
 10.5 MPa
@Strain 2.00 %
ISO 604 (10)
 17.0 MPa
@Strain 5.00 %
ISO 604 (10)
Charpy Impact, Notched 107 kJ/m²Partial Break; ISO 179-1/1eA
 128 kJ/m²Double Notched
 
Electrical PropertiesOriginal ValueComments
Surface Resistivity per Square 1.00e+13 ohmANSI/ESD STM 11.11
 
Thermal PropertiesOriginal ValueComments
CTE, linear 94.0 µin/in-°FASTM E-831 (TMA)
 230 µm/m-°C
@Temperature 23.0 - 100 °C
Melting Point 280 °FASTM D3418
Deflection Temperature at 1.8 MPa (264 psi) 84.0 °FASTM D648
Minimum Service Temperature, Air -150 °C
 
Chemical Resistance PropertiesOriginal ValueComments
Acids, Strong (pH 1-3) Acceptable
Acids, Weak Acceptable
Alcohols Acceptable
Alkalies, Strong (pH 11-14) Acceptable
Alkalies, Weak Acceptable
Chlorinated Solvents Acceptable
Continuous Sunlight Limited
Hot Water / Steam Limited
Hydrocarbons - Aliphatic Acceptable
Hydrocarbons - Aromatic Acceptable
Inorganic Salt Solutions Acceptable
Ketones, Esters Acceptable
 
Descriptive Properties
ESd categoryInsulative

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.