Mitsubishi Chemical Advanced Materials Sultron™ LSG PSU Extruded, Unfilled, Polysulfone
Categories: Polymer; Thermoplastic; Polysulfone (PSU)

Material Notes: Life Science Grade PSU stock shapes made from unfilled Udel™ PSU resin. Pre-assessed for biocompatibility on both resin and shape for up to 24 hours contact with body tissue according to USP VI and ISO 10993 and wetted contact in bioprocessing. Good hydrolysis resistance as well as great mechanical, thermal, and electrical properties.

Printer friendly version Printer friendly version  PDF Download Download as PDF  Add to Folder:
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.24 g/cc1.24 g/ccASTM D792
Water Absorption at Saturation 0.600 %0.600 %ASTM D570 (17)
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 89.089.0ASTM D785
Hardness, Shore D 80.080.0ISO 868
Tensile Strength 88.0 MPa12800 psiISO 527-1/-2 (7)
Elongation at Yield 5.00 %5.00 %ISO 527-1/-2 (7)
Flexural Strength 120 MPa17400 psiISO 178 (12)
Compressive Yield Strength  25.0 MPa
@Strain 1.00 %
3630 psi
@Strain 1.00 %
ISO 604 (10)
 49.0 MPa
@Strain 2.00 %
7110 psi
@Strain 2.00 %
ISO 604 (10)
 101 MPa
@Strain 5.00 %
14600 psi
@Strain 5.00 %
ISO 604 (10)
Shear Strength 62.0 MPa8990 psiASTM D732
Charpy Impact, Notched 0.350 J/cm²1.67 ft-lb/in²ISO 179-1/1eA
 
Electrical PropertiesMetricEnglishComments
Surface Resistivity per Square 1.00e+14 ohm1.00e+14 ohmANSI/ESD STM 11.11
Dielectric Constant 3.14
@Frequency 1.00e+6 Hz
3.14
@Frequency 1.00e+6 Hz
ASTM D150
Dielectric Strength 16.7 kV/mm425 kV/inASTM D149
 30.0 kV/mm762 kV/inIEC 60243-1 (15)
Dissipation Factor 0.000800
@Frequency 1.00e+6 Hz
0.000800
@Frequency 1.00e+6 Hz
ASTM D150
 
Thermal PropertiesMetricEnglishComments
CTE, linear 55.8 µm/m-°C31.0 µin/in-°FASTM E-831 (TMA)
 55.0 µm/m-°C
@Temperature 23.0 - 100 °C
30.6 µin/in-°F
@Temperature 73.4 - 212 °F
 55.0 µm/m-°C
@Temperature 23.0 - 150 °C
30.6 µin/in-°F
@Temperature 73.4 - 302 °F
 70.0 µm/m-°C
@Temperature >=150 °C
38.9 µin/in-°F
@Temperature >=302 °F
Thermal Conductivity 0.259 W/m-K1.80 BTU-in/hr-ft²-°F
 0.260 W/m-K1.80 BTU-in/hr-ft²-°F
Maximum Service Temperature, Air 149 °C300 °FContinuous Use Temperature in Air after 20000 hr
Deflection Temperature at 1.8 MPa (264 psi) 171 °C340 °FASTM D648
Minimum Service Temperature, Air -50.0 °C-58.0 °F
Glass Transition Temp, Tg 190 °C374 °FDMA- Tan d
 
Compliance PropertiesMetricEnglishComments
USP Class VI YesYes
 
Chemical Resistance PropertiesMetricEnglishComments
Acids, Strong (pH 1-3) UnacceptableUnacceptable
Acids, Weak AcceptableAcceptable
Alcohols AcceptableAcceptable
Alkalies, Strong (pH 11-14) UnacceptableUnacceptable
Alkalies, Weak AcceptableAcceptable
Chlorinated Solvents UnacceptableUnacceptable
Continuous Sunlight LimitedLimited
Hot Water / Steam LimitedLimited
Hydrocarbons - Aliphatic LimitedLimited
Hydrocarbons - Aromatic UnacceptableUnacceptable
Inorganic Salt Solutions AcceptableAcceptable
Ketones, Esters UnacceptableUnacceptable
 
Miscellaneous PropertiesMetricEnglishComments
Targeted Usage Structural UsesStructural Uses
 
Descriptive Properties
ESd categoryInsulative

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.